Weld Heat Input and Carbon Equivalent Preheat Calculator
At 26 V, 220 A, and 300 mm/min (11.8 in/min) travel speed using GMAW (MIG/MAG, thermal efficiency k = 0.8), the linear arc energy is E = 1.14 kJ/mm and the true thermal heat input is Q = 0.915 kJ/mm (23.2 kJ/in). For a 25 mm (1 in) Hardox 450 wear plate (CE_IIW = 0.47, CET = 0.33) welded with H5 extra-low-hydrogen wire, the minimum preheat temperature is 125 °C (257 °F) with a strict maximum interpass temperature of 225 °C (437 °F) to yield a t8/5 cooling time of 4.8 s and prevent Heat-Affected Zone (HAZ) softening.
Interactive Weld Heat Input, Carbon Equivalent and Preheat Temperature Calculator
Welding Procedure (WPS), Base Steel & Chemistry Inputs
Fast cooling rate on thick plate traps diffusible hydrogen in a hard martensitic HAZ (>380–420 HV), risking delayed cold toe/underbead cracking 24–48 hours after welding. Verify preheat Tp and use H4/H5 consumables.
Click Load on any structural, Q&T, Hardox/AR wear plate, or alloy steel row to populate chemistry and thickness into the calculator.
Q & t8/5 Window
Filler Wire / Electrode
Action
SSAB Hardox 450 (12 mm)
12 mm bucket cheek liner & wear strip fillet
12 mm (0.47 in)
CE 0.47 · CET 0.33 · Pcm 0.29
20 °C (68 °F)
225 °C (437 °F)
0.6–1.5 kJ/mm
t8/5: 5–20 s
ER70S-6 / E8018-C3 H4
SSAB Hardox 400 (15 mm)
15 mm dump body floor & loader bucket wrapper
15 mm (0.59 in)
CE 0.43 · CET 0.30 · Pcm 0.26
20 °C (68 °F)
225 °C (437 °F)
0.6–1.6 kJ/mm
t8/5: 5–20 s
ER70S-6 / E7018 H4 (under-matched)
ASTM A36 / S235JR (16 mm)
16 mm general structural brackets & tank mounts
16 mm (0.63 in)
CE 0.38 · CET 0.28 · Pcm 0.24
20 °C (68 °F)
250 °C (482 °F)
0.8–2.5 kJ/mm
t8/5: 8–25 s
ER70S-6 / E7018 (H8)
EN S355J2 / A572 Gr50 (20 mm)
20 mm excavator boom side plate & chassis web
20 mm (0.79 in)
CE 0.45 · CET 0.33 · Pcm 0.27
50 °C (122 °F)
250 °C (482 °F)
0.9–2.2 kJ/mm
t8/5: 8–25 s
ER70S-6 / E7018-1 H4R
EN S690QL / Strenx 700 (20 mm)
20 mm crane boom shell & lowboy trailer gooseneck
20 mm (0.79 in)
CE 0.55 · CET 0.35 · Pcm 0.29
100 °C (212 °F)
225 °C (437 °F)
0.6–1.5 kJ/mm
t8/5: 5–20 s
ER110S-G / E11018-M H4
Generic AR400 Wear Plate (20 mm)
20 mm aggregate hopper & bucket bottom wear plate
20 mm (0.79 in)
CE 0.54 · CET 0.37 · Pcm 0.32
125 °C (257 °F)
200 °C (392 °F)
0.7–1.5 kJ/mm
t8/5: 5–20 s
ER70S-6 / E7018-1 H4R
Generic AR500 Wear Plate (20 mm)
20 mm high-carbon abrasion liner & impact pad
20 mm (0.79 in)
CE 0.73 · CET 0.50 · Pcm 0.44
150 °C (302 °F)
175 °C (347 °F)
0.6–1.2 kJ/mm
t8/5: 5–15 s
ER309L / ER307 Stainless Buffer
SSAB Hardox 450 (25 mm)
25 mm heavy rock bucket side cutter & heel shroud
25 mm (0.98 in)
CE 0.47 · CET 0.33 · Pcm 0.29
125 °C (257 °F)
225 °C (437 °F)
0.7–1.6 kJ/mm
t8/5: 5–20 s
ER70S-6 / E8018-C3 H5
SSAB Hardox 500 (25 mm)
25 mm quarry loader lip & granite chute liner
25 mm (0.98 in)
CE 0.66 · CET 0.45 · Pcm 0.40
150 °C (302 °F)
175 °C (347 °F)
0.6–1.3 kJ/mm
t8/5: 5–15 s
E7018-1 H4R / ER307 Austenitic
Hadfield Mn13 (12% Mn) Austenitic (25 mm)
25 mm jaw crusher plate & manganese impact bar
25 mm (0.98 in)
CE 3.28 · CET 2.41 · Pcm 1.80
20 °C (68 °F)
100 °C (212 °F)
0.5–1.0 kJ/mm
t8/5: Fast Cool (<5 s)
ER307 / E308Mo-16 — NEVER PREHEAT
EN S690QL / ASTM A514 T-1 (35 mm)
35 mm mining shovel stick & outrigger box beam
35 mm (1.38 in)
CE 0.55 · CET 0.35 · Pcm 0.29
150 °C (302 °F)
225 °C (437 °F)
0.7–1.6 kJ/mm
t8/5: 5–20 s
ER110S-G / E11018-M H4
30MnB5 Boron Base Cutting Edge (35 mm)
35 mm weld-in excavator bucket lip & dozer edge
35 mm (1.38 in)
CE 0.57 · CET 0.45 · Pcm 0.40
175 °C (347 °F)
225 °C (437 °F)
0.7–1.5 kJ/mm
t8/5: 6–18 s
E7018-1 H4R / ER70S-6 Low-H2
EN S355J2 / A572 Gr50 (40 mm)
40 mm heavy carbody bearing ring & boom foot lug
40 mm (1.57 in)
CE 0.45 · CET 0.33 · Pcm 0.27
100 °C (212 °F)
250 °C (482 °F)
1.0–2.5 kJ/mm
t8/5: 8–25 s
E7018-1 H4R / E71T-1M H4
AISI 4140 / 42CrMo4 Q&T Boss (40 mm)
40 mm weld-on pin boss & forged tooth adapter nose
40 mm (1.57 in)
CE 0.78 · CET 0.56 · Pcm 0.51
250 °C (482 °F)
350 °C (662 °F)
0.9–1.8 kJ/mm
t8/5: 10–30 s
E8018-B2 / ER80S-D2 + Slow Cool Blanket
SSAB Hardox 450 (12 mm)
12 mm bucket cheek liner & wear strip fillet
CE 0.47 · CET 0.33
Min Preheat Tp
20 °C (68 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.6–1.5 kJ/mm (5–20 s)
Consumable
ER70S-6 / E8018-C3 H4
SSAB Hardox 400 (15 mm)
15 mm dump body floor & loader bucket wrapper
CE 0.43 · CET 0.30
Min Preheat Tp
20 °C (68 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.6–1.6 kJ/mm (5–20 s)
Consumable
ER70S-6 / E7018 H4 (under-matched)
ASTM A36 / S235JR (16 mm)
16 mm general structural brackets & tank mounts
CE 0.38 · CET 0.28
Min Preheat Tp
20 °C (68 °F)
Max Interpass
250 °C (482 °F)
Heat Input Window
0.8–2.5 kJ/mm (8–25 s)
Consumable
ER70S-6 / E7018 (H8)
EN S355J2 / A572 Gr50 (20 mm)
20 mm excavator boom side plate & chassis web
CE 0.45 · CET 0.33
Min Preheat Tp
50 °C (122 °F)
Max Interpass
250 °C (482 °F)
Heat Input Window
0.9–2.2 kJ/mm (8–25 s)
Consumable
ER70S-6 / E7018-1 H4R
EN S690QL / Strenx 700 (20 mm)
20 mm crane boom shell & lowboy trailer gooseneck
CE 0.55 · CET 0.35
Min Preheat Tp
100 °C (212 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.6–1.5 kJ/mm (5–20 s)
Consumable
ER110S-G / E11018-M H4
Generic AR400 Wear Plate (20 mm)
20 mm aggregate hopper & bucket bottom wear plate
CE 0.54 · CET 0.37
Min Preheat Tp
125 °C (257 °F)
Max Interpass
200 °C (392 °F)
Heat Input Window
0.7–1.5 kJ/mm (5–20 s)
Consumable
ER70S-6 / E7018-1 H4R
Generic AR500 Wear Plate (20 mm)
20 mm high-carbon abrasion liner & impact pad
CE 0.73 · CET 0.50
Min Preheat Tp
150 °C (302 °F)
Max Interpass
175 °C (347 °F)
Heat Input Window
0.6–1.2 kJ/mm (5–15 s)
Consumable
ER309L / ER307 Stainless Buffer
SSAB Hardox 450 (25 mm)
25 mm heavy rock bucket side cutter & heel shroud
CE 0.47 · CET 0.33
Min Preheat Tp
125 °C (257 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.7–1.6 kJ/mm (5–20 s)
Consumable
ER70S-6 / E8018-C3 H5
SSAB Hardox 500 (25 mm)
25 mm quarry loader lip & granite chute liner
CE 0.66 · CET 0.45
Min Preheat Tp
150 °C (302 °F)
Max Interpass
175 °C (347 °F)
Heat Input Window
0.6–1.3 kJ/mm (5–15 s)
Consumable
E7018-1 H4R / ER307 Austenitic
Hadfield Mn13 (12% Mn) Austenitic (25 mm)
25 mm jaw crusher plate & manganese impact bar
CE 3.28 · CET 2.41
Min Preheat Tp
20 °C (68 °F)
Max Interpass
100 °C (212 °F)
Heat Input Window
0.5–1.0 kJ/mm (Fast Cool (<5 s))
Consumable
ER307 / E308Mo-16 — NEVER PREHEAT
EN S690QL / ASTM A514 T-1 (35 mm)
35 mm mining shovel stick & outrigger box beam
CE 0.55 · CET 0.35
Min Preheat Tp
150 °C (302 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.7–1.6 kJ/mm (5–20 s)
Consumable
ER110S-G / E11018-M H4
30MnB5 Boron Base Cutting Edge (35 mm)
35 mm weld-in excavator bucket lip & dozer edge
CE 0.57 · CET 0.45
Min Preheat Tp
175 °C (347 °F)
Max Interpass
225 °C (437 °F)
Heat Input Window
0.7–1.5 kJ/mm (6–18 s)
Consumable
E7018-1 H4R / ER70S-6 Low-H2
EN S355J2 / A572 Gr50 (40 mm)
40 mm heavy carbody bearing ring & boom foot lug
CE 0.45 · CET 0.33
Min Preheat Tp
100 °C (212 °F)
Max Interpass
250 °C (482 °F)
Heat Input Window
1.0–2.5 kJ/mm (8–25 s)
Consumable
E7018-1 H4R / E71T-1M H4
AISI 4140 / 42CrMo4 Q&T Boss (40 mm)
40 mm weld-on pin boss & forged tooth adapter nose
CE 0.78 · CET 0.56
Min Preheat Tp
250 °C (482 °F)
Max Interpass
350 °C (662 °F)
Heat Input Window
0.9–1.8 kJ/mm (10–30 s)
Consumable
E8018-B2 / ER80S-D2 + Slow Cool Blanket
EN 1011-2
How Thermal Heat Input (Q = k·E), Carbon Equivalent (CE / CET / Pcm), Preheat & t8/5 Cooling Time Are Calculated
Welding quenched-and-tempered wear plates (Hardox 450/500, AR400/500) and high-yield boom steels (S690QL / Strenx 700 / A514) requires balancing two opposing failure modes: cooling too fast causes delayed hydrogen cold cracking, while cooling too slowly over-tempers and softens the Heat-Affected Zone (HAZ).
Per ISO/TR 17671-1 and EN 1011-1, linear arc energy E is multiplied by the arc thermal efficiency factor k (0.8 for GMAW, FCAW, SMAW; 1.0 for SAW; 0.6 for GTAW) to obtain true thermal heat input Q:
E (kJ/mm) = (V × I × 60) / (1,000 × v_mm/min)
Q (kJ/mm) = k × E | Q (kJ/in) = 25.4 × Q (kJ/mm)
CE_IIW = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15
CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40
Pcm = C + Si/30 + (Mn+Cu+Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B
2. EN 1011-2 Method B Preheat (Tp) & 2D/3D t8/5 Cooling Time
Minimum preheat temperature T_p under EN 1011-2 Method B combines CET, combined joint heat-sink thickness d_comb, diffusible hydrogen H_D (ml/100g), and heat input Q, followed by 2D thin-plate or 3D thick-plate cooling time t8/5 from 800 °C to 500 °C:
Defines arc thermal efficiency factors k (GMAW/FCAW/SMAW = 0.8, SAW = 1.0, GTAW = 0.6), Method A (CE_IIW) and Method B (CET) preheat temperature calculation, combined thickness d_comb, and 2D/3D t8/5 cooling time equations.
International Organization for Standardization (ISO)
International adoption of CET carbon equivalent, diffusible hydrogen scale (HD in ml/100g), heat input window, and cooling time t8/5 from 800 °C to 500 °C for high-strength structural and quenched-and-tempered steels.
Specifies minimum preheat and interpass temperatures (Table 5.8) and alternative hydrogen control / Ito-Bessyo Pcm crack susceptibility index for low-carbon high-strength and quenched-and-tempered steels.
Authoritative OEM guidelines for Hardox 400, Hardox 450, Hardox 500, and Strenx 700 (S690QL), defining maximum interpass temperatures (175 °C–225 °C) and recommended t8/5 cooling time windows (5–20 s) to prevent HAZ over-tempering.
What is the difference between Arc Energy (E) and Thermal Heat Input (Q) under ISO/TR 17671-1 and EN 1011-1?
Arc energy E = (V × I × 60) / (1,000 × v) measures raw electrical power per millimeter of weld travel, whereas true thermal heat input Q = k × E multiplies arc energy by the process thermal efficiency factor k (0.8 for GMAW/MIG, FCAW, and SMAW stick; 1.0 for Submerged Arc SAW; and 0.6 for GTAW/TIG). European WPS specs (EN ISO 15614-1) require applying k, whereas older AWS D1.1 procedures historically reported unfactored arc energy (k = 1.0).
When should I use CE(IIW) versus CET (EN 1011-2) or Pcm (AWS D1.1 Annex H) for carbon equivalent?
Use CE(IIW) = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 for classical carbon-manganese structural steels with carbon C > 0.18% (such as A36 and S355J2). For modern low-carbon micro-alloyed Q&T wear plates and high-yield steels (Hardox 450, S690QL / Strenx 700, Boron 30MnB5) where C is 0.14%–0.22% with trace Boron, CET (EN 1011-2 Method B) and Ito-Bessyo Pcm (AWS D1.1 Annex H) accurately capture the higher weight of carbon and boron without over-penalizing alloying additions.
Why does Hardox 450 / 500 have a strict maximum interpass temperature (175 °C–225 °C) and t8/5 cooling limit?
Hardox 400, 450, and 500 gain their 400–500 HBW abrasion resistance from a quenched martensitic microstructure tempered at ~200 °C–250 °C at the steel mill. If preheat/interpass temperature exceeds 225 °C (Hardox 450) or 175 °C (Hardox 500), or if excessive heat input Q > 1.8 kJ/mm causes the 800 °C-to-500 °C cooling time t8/5 to exceed 20 seconds, the Heat-Affected Zone (HAZ) over-tempers into soft ferrite-pearlite (~260 HBW) and loses wear life or cracks beside the weld toe.
How do you weld an AISI 4140 (42CrMo4) pin boss or forged tooth adapter onto an S355 excavator boom or bucket?
AISI 4140 has a very high carbon equivalent (CE_IIW ≈ 0.78, CET ≈ 0.56) that forms brittle untempered martensite (>550 HV) if welded cold. Preheat the 4140 boss to 225 °C–260 °C (437 °C–500 °F), use strictly H4 extra-low-hydrogen consumables (E8018-C3 H4R or ER70S-6 / E7018-1 buttering layer), maintain interpass below 350 °C, peen multi-pass beads, and wrap the joint in a ceramic thermal blanket for slow post-weld cooling.
Why must you NEVER preheat Hadfield Mn13 (11%–14% Austenitic Manganese) crusher liners or bucket impact bars?
Unlike ferritic carbon steels, Hadfield Mn13 (ASTM A128 / X120Mn12) is an austenitic work-hardening steel. Heating Mn13 above 260 °C (500 °F) causes brittle manganese carbides to precipitate along austenitic grain boundaries, leading to catastrophic spalling and cracking under impact. Always weld Hadfield manganese steel with ZERO preheat, low heat input (Q < 1.0 kJ/mm), ER307/308Mo stainless filler, and strict interpass temperature ≤ 100 °C (212 °F).
Shop bench
Related Free Heavy Equipment Shop Tools
Free shop calculators grounded in published standards (Parker Catalog 4300, SAE J1939, AS568). They run in the browser with no login and no paywall.
Need the Exact Factory Schematic or Torque Table for This Machine?
Stop scrolling through 1,200 to 4,000-page OEM PDFs on a phone screen. Upload your shop's Service and Test & Adjust manuals into Rigovely's isolated Scoped OEM Index. The Beta diagnostic co-pilot pinpoints the wiring pinout, relief pressure, or torque sequence by S/N prefix alongside Fleetio, SAP, or Maximo.